ASTM A209
This standard specification for seamless carbon-molybdenum alloy-steel boiler and superheater tubes
This specification covers several grades of minimum wall thickness, seamless, carbon-molybdenum alloy steel, boiler and superheater tubes.
This standard has three kinds of steel grade: Grade T1, Grade T1a, Grade T1b
This specification covers tubes ½ to 5 in (12.7 to 127) mm in outside diameter, and 0.035 to 0.500 in (0.9 to 12.7) mm in wall thickness .
Reference Standard:
ASTM A450/A450M specification for general requirements for carbon, Ferritic Alloy and Austenitic alloy steel tubes.
Chemical composition:
| C % | Mn % | P % | S % | Si % | Mo % | |
| Gr. T1 | 0.10 – 0.20 | 0.30 – 0.80 | Max:0.025 | Max:0.025 | 0.10 – 0.50 | 0.44 – 0.65 |
| Gr. T1a | 0.15 – 0.25 | 0.30 – 0.80 | Max:0.025 | Max:0.025 | 0.10 – 0.50 | 0.44 – 0.65 |
| Gr. T1b | Max: 0.14 | 0.30 – 0.80 | Max:0.025 | Max:0.025 | 0.10 – 0.50 | 0.44 – 0.65 |
Mechanical property:
| Tensile Strength, KSI (MPA) | Yield Strength, KSI (MPA) | |
| Gr. T1 | 55 (380) | 30 (205) |
| Gr. T1a | 60 (415) | 32 (220) |
| Gr. T1b | 53 (365) | 28 (195) |
Elongation:
This table gives the computed minimum values:
| Wall Thickness | Wall Thickness | Elongation in 2in, or 50 mm |
| In | mm | min, % |
| 0.312 (5/16) | 8 | 30 |
| 0.281 (9/32) | 7.2 | 29 |
| 0.250 (1/4) | 6.4 | 27 |
| 0.219 (7/32) | 5.6 | 26 |
| 0.188 (3/16) | 4.8 | 24 |
| 0.165 (5/32) | 4 | 22 |
| 0.125 (1/8) | 3.2 | 21 |
| 0.094 (3/32) | 2.4 | 20 |
| 0.062 (1/16) | 1.6 | 18 |
Hardness:
| Brinell Hardness number (tubes 0.20 in, (5.1) mm and over in wall thickness) | Rockwell Hardness number (tubes less than 0.20 in,(5.1)mm in wall thickness) | |
| Grade t1 | 146 | B80 |
| Grade T1a | 153 | B81 |
| Grade T1b | 137 | B77 |
Heat treatment:
Hot-finished tubes shall be heat treated at temperature of 1200°F (650°C)or higher, Cold-finished tubes shall after final cold finishing, be heat treated at temperature of 1200°F (650°C) or higher, or tubing may be furnished in tempered condition, if furnished in the normalized and tempered condition, the minimum tempering temperature shall be 1200°F (650°C).