ASTM A334

This standard specification for seamless and welded carbon and alloy-steel tubes for low-temperature service.

This specification covers several grades of minimum wall-thickness seamless and welded carbon and alloy-steel tubes intended for use at low temperatures. Some product sizes may not be available under this specification because heavier wall thickness have an adverse effect on low temperature impact properties.

This standard has many steel grades: Gr.1, Gr.3, Gr.6, Gr.7, Gr.8, Gr.9, Gr.11

Reference standard:

ASTM A450/A450 M specification for general requirements for carbon, ferritic alloy, and austenitic alloy steel tubes.

Chemical Composition:

  C %, max Mn % P %, max S %, max Si % Ni % Cr % Cu % Co% Mo %
Gr.1 0.30 0.4-1.06 0.025 0.025 —- —- —- —- —- —-
Gr.3 0.19 0.31-0.64 0.025 0.025 0.18-0.37 3.18-3.82 —- —- —- —-
Gr.6 0.30 0.29-1.06 0.025 0.025 0.10 min —- —- —- —- —-
Gr.7 0.19 0.90 max 0.025 0.025 0.13-0.32 2.03-2.57 —- —- —- —-
Gr.8 0.13 0.90 max 0.025 0.025 0.13-0.32 8.40-9.60 —- —- —- —-
Gr.9 0.20 0.40-1.06 0.025 0.025 —- 1.60-2.24 —- 0.75-1.25 —- —–
Gr.11 0.10 0.60, max 0.025 0.025 0.35, max 35.0-37.0 0.50, max —- 0.50, max 0.50, max

Mechanical Property:

  Grade 1 Grade 3 Grade 6 Grade 7 Grade 8 Grade 9 Grade 11
TS, min 380 450 415 450 690 435 450
YS, min 205 240 240 240 520 315 240
hardness 163 HB 190 HB 190 HB 190 HB 190 HB 190 HB 190 HB