ASTM A209

This standard specification for seamless carbon-molybdenum alloy-steel boiler and superheater tubes

This specification covers several grades of minimum wall thickness, seamless, carbon-molybdenum alloy steel, boiler and superheater tubes.

This standard has three kinds of steel grade: Grade T1, Grade T1a, Grade T1b

This specification covers tubes ½ to 5 in (12.7 to 127) mm in outside diameter, and 0.035 to 0.500 in (0.9 to 12.7) mm in wall thickness .

Reference Standard:

ASTM A450/A450M specification for general requirements for carbon, Ferritic Alloy and Austenitic alloy steel tubes.

Chemical composition:

  C % Mn % P % S % Si % Mo %
Gr. T1 0.10 – 0.20 0.30 – 0.80 Max:0.025 Max:0.025 0.10 – 0.50 0.44 – 0.65
Gr. T1a 0.15 – 0.25 0.30 – 0.80 Max:0.025 Max:0.025 0.10 – 0.50 0.44 – 0.65
Gr. T1b Max: 0.14 0.30 – 0.80 Max:0.025 Max:0.025 0.10 – 0.50 0.44 – 0.65

Mechanical property:

  Tensile Strength, KSI (MPA) Yield Strength, KSI (MPA)
Gr. T1 55 (380) 30 (205)
Gr. T1a 60 (415) 32 (220)
Gr. T1b 53 (365) 28 (195)

Elongation:

This table gives the computed minimum values:

Wall Thickness Wall Thickness Elongation in 2in, or 50 mm
In mm min, %
0.312 (5/16) 8 30
0.281 (9/32) 7.2 29
0.250 (1/4) 6.4 27
0.219 (7/32) 5.6 26
0.188 (3/16) 4.8 24
0.165 (5/32) 4 22
0.125 (1/8) 3.2 21
0.094 (3/32) 2.4 20
0.062 (1/16) 1.6 18

Hardness:

  Brinell Hardness number (tubes 0.20 in, (5.1) mm and over in wall thickness) Rockwell Hardness number (tubes less than 0.20 in,(5.1)mm in wall thickness)
Grade t1 146 B80
Grade T1a 153 B81
Grade T1b 137 B77

Heat treatment:

Hot-finished tubes shall be heat treated at temperature of 1200°F (650°C)or higher, Cold-finished tubes shall after final cold finishing, be heat treated at temperature of 1200°F (650°C) or higher, or tubing may be furnished in tempered condition, if furnished in the normalized and tempered condition, the minimum tempering temperature shall be 1200°F (650°C).